Stainless Steel Grade Selection Guide · Hardness · Heat Treatment · Corrosion · Procurement Control
420 vs 304 Stainless Steel: Hardness, Heat Treatment, Corrosion & Selection Guide
How to choose between a heat-treatable martensitic stainless steel and a highly fabricable austenitic stainless steel by failure mode, delivery condition and verification requirements
Comparing 420 vs 304 stainless steel is not a matter of ranking one grade above the other. The two alloys belong to different metallurgical families and are designed to solve different engineering problems. 420 is selected when hardness, wear resistance, edge retention or heat-treated strength controls performance. 304 is selected when corrosion resistance, weldability, formability, toughness and cleanability control performance.
This distinction has an important purchasing consequence: the grade name alone is not enough. A 420 component can be supplied annealed for machining, hardened and tempered to a specified Rockwell hardness, or produced from a higher- or lower-carbon martensitic subgrade. A 304 component can be annealed, heavily cold worked, welded, polished or passivated, and each condition changes its mechanical and fabrication behavior.
Buyers should therefore begin with the expected failure mode. Will the part lose function because a cutting edge becomes dull, a shaft wears, a welded joint cracks, the surface corrodes, a deep-drawn shell splits, or the delivered hardness misses the drawing requirement? Once that question is clear, 420 and 304 stop looking like interchangeable “stainless steel” options.
This guide explains the metallurgical difference, heat-treatment logic, realistic hardness comparison, corrosion limits, welding and machining behavior, subgrade traps, application selection, alternative grades, MTC and PMI verification, and the RFQ information required to buy the correct condition—not merely the correct alloy name.

Quick Answer: Should You Choose 420 or 304 Stainless Steel?
Buyer Decision Rule
Choose 420 when the drawing requires a heat-treated hardness, cutting edge, wear surface, high-strength martensitic condition or polished hard component. Choose 304 or 304L when the part must be formed, welded, cleaned repeatedly or exposed to a general wet environment where corrosion resistance and fabrication reliability matter more than high hardness.
| Requirement | Better Starting Choice | Why | Buyer Caution |
|---|---|---|---|
| High Rockwell hardness | 420 or another hardenable stainless | Martensitic 420 responds to hardening and tempering. | Specify the exact subgrade, heat-treatment condition and HRC acceptance range. |
| Knife or cutting edge | 420-family / higher-carbon martensitic grade | Hardness and edge retention are available after heat treatment. | “420” alone may not define enough carbon for the required edge performance. |
| Wear-resistant shaft or valve component | 420 as a starting point | Hardened martensitic structure provides better wear resistance than annealed 304. | Review toughness, corrosion severity and distortion after heat treatment. |
| Deep drawing or complex sheet forming | 304 | Austenitic 304 offers high ductility and excellent formability. | Cold work increases strength and can increase magnetic response. |
| Welded food or process equipment | 304L / 316L depending environment | Austenitic grades are much easier to weld and fabricate. | Use 316L instead when chlorides or more aggressive chemistry require additional corrosion margin. |
| General wet-service corrosion resistance | 304 | Its alloy design gives stronger general corrosion performance than ordinary 420. | 304 is not a seawater or severe-chloride solution. |
| Hardness plus stronger corrosion margin | 431, 440-series, 17-4PH or specialty grade | Another alloy may balance hardness, strength and corrosion more effectively. | Do not force either 420 or 304 into an application outside its design envelope. |
The key point is that 420 and 304 are normally not direct substitutes. If the drawing calls for HRC after heat treatment, 304 usually cannot satisfy the functional requirement. If the equipment requires extensive welding, deep forming and reliable wet-service corrosion resistance, ordinary 420 usually creates avoidable fabrication and maintenance risk.
Why 420 and 304 Are Fundamentally Different Stainless Steels
420 is martensitic: its performance is created by heat treatment
Type 420 belongs to the martensitic stainless family. Its chromium content provides stainless behavior, while its higher carbon content enables transformation to a hard martensitic structure after austenitizing and quenching. Tempering is then used to adjust the final balance between hardness, strength, toughness and dimensional stability.
This means a statement such as “420 has high strength” is incomplete. Annealed 420 is intentionally softer so it can be machined or formed more easily. The same alloy can become much harder after an appropriate hardening cycle. For purchasing, delivery condition is part of the material definition.
304 is austenitic: its value comes from corrosion resistance and fabrication
Type 304 is a chromium-nickel austenitic stainless steel. It is widely used because its austenitic structure remains ductile and tough, supports deep drawing and bending, and can be welded by conventional stainless-steel processes without the same hard heat-affected-zone behavior associated with martensitic grades.
304 does work harden substantially during cold deformation, so strength can increase through rolling, drawing or forming. However, it is not hardened by the same conventional quench-and-temper route used for 420. A cold-worked 304 strip therefore should not be treated as a functional equivalent to a properly hardened 420 blade or wear component.
| Factor | 420 Stainless Steel | 304 Stainless Steel | Practical Consequence |
|---|---|---|---|
| Metallurgical family | Martensitic | Austenitic | The two grades respond differently to heat treatment, welding and forming. |
| Primary design priority | Hardness, strength, wear and edge retention | Corrosion resistance, ductility and fabrication | Selection should follow the dominant failure mode. |
| Conventional quench hardening | Yes | No | 420 can be supplied soft and later hardened to a specified condition. |
| Cold-work strengthening | Possible, but not the main hardening route | Strong response | Cold-worked 304 can become strong but remains a different material solution. |
| General weldability | More difficult | Excellent | 420 often needs tighter thermal control around welding. |
| General corrosion margin | Moderate and condition-sensitive | Higher in many common environments | 304 is usually the safer starting point for wet general fabrication. |
Chemistry and Microstructure: Why Carbon, Chromium and Nickel Matter
The chemistry difference explains most of the practical behavior. Type 420 uses a chromium-rich composition with substantially more carbon than 304. Type 304 uses more chromium together with significant nickel and relatively low carbon.

| Element | 420 Family | 304 Family | Engineering Meaning |
|---|---|---|---|
| Carbon | Significantly higher; exact range depends on specification/subgrade | Low; standard 304 commonly allows up to 0.08% | Higher carbon gives 420 its hardening potential but makes welding and corrosion control more condition-sensitive. |
| Chromium | Typically in the low-teens range | Typically around 18–20% | Chromium supports passive-film formation; usable chromium can also be affected by carbide formation. |
| Nickel | Low or not a major intentional addition in standard Type 420 | Significant, commonly around the 8–10.5% range under common specifications | Nickel stabilizes the austenitic structure and supports ductility and fabrication behavior. |
| Molybdenum | Not the defining addition in ordinary Type 420 | Not the defining addition in ordinary Type 304 | If chloride pitting resistance is the problem, 316L or a higher-alloy grade may be more appropriate. |
These are selection-level descriptions rather than purchase limits. Exact chemistry must be checked against the governing ASTM, EN, JIS, GB or customer specification and the heat-specific MTC.
More carbon does not simply mean “better 420”
Higher carbon can increase attainable hardness because more carbon is available to participate in the hardened martensitic structure and carbide population. But the trade-off can include lower toughness, more demanding heat treatment, reduced weldability and potentially lower corrosion margin if the microstructure or heat treatment is not well controlled.
Therefore, a buyer should not automatically request the highest-carbon 420-family material. The correct carbon level depends on the required hardness, edge geometry, section thickness, impact load, corrosion environment and heat-treatment capability.
420 Designation Map: Similar Names Do Not Mean Automatic Equivalence
Important Procurement Warning
“AISI 420,” “SUS420J1,” “SUS420J2,” “X20Cr13,” “X30Cr13,” “X46Cr13” and “420HC” should not be treated as automatic one-to-one equivalents. They belong to the same broad martensitic chromium-steel space, but carbon limits, mechanical requirements, heat treatment and product standards can differ.
| Name | Standard / Region | What It Tells the Buyer | What Still Needs Verification |
|---|---|---|---|
| Type 420 / UNS S42000 | ASTM / North American designation family | Heat-treatable martensitic chromium stainless steel. | Applicable product specification, chemistry, condition and target hardness. |
| SUS420J1 | JIS | Lower-carbon 420-family martensitic grade. | Do not substitute for J2 or a higher-carbon grade when HRC/edge performance is critical. |
| SUS420J2 | JIS | Higher-carbon 420-family grade often used where greater hardness is required. | Heat-treatment route, hardness range and dimensional control. |
| 1.4021 / X20Cr13 | EN | Martensitic chromium grade in a similar application space. | Not an automatic dimensional/chemical equivalent to every “420” specification. |
| 1.4028 / X30Cr13 | EN | Higher-carbon martensitic chromium grade. | Required hardness, toughness and governing product standard. |
| 1.4034 / X46Cr13 | EN | Higher-carbon martensitic grade commonly associated with cutting applications. | Do not approve solely on a generic “420 equivalent” statement. |
| 420HC | Commercial / trade usage | Usually indicates a higher-carbon 420-type material. | There is no single universal chemistry implied by the letters “HC”; require the producer specification and MTC. |
| 304 / UNS S30400 | ASTM / common global designation | General-purpose austenitic Cr-Ni stainless steel. | Product standard, condition, surface and dimensions. |
| 304L / UNS S30403 | ASTM / common global designation | Low-carbon 304-family grade for welded corrosion-resistant fabrication. | Confirm whether dual certification is acceptable under the project specification. |
For hardness-critical martensitic material, the safest PO identifies the exact designation and product standard, then adds delivery condition and final hardness. An “equivalent grade” should be approved only after chemistry, heat treatment, mechanical properties, dimensional requirements and application function have been compared.
Heat Treatment: The Most Important Difference Between 420 and 304
420 performance is created through a heat-treatment sequence
A common 420 manufacturing route is: machine or form the part in a softer condition, austenitize at a grade-appropriate temperature, quench to form martensite, and temper to reach the required combination of hardness and toughness. The exact cycle depends on the 420 subgrade, product form, section size, furnace atmosphere and dimensional requirements.

Do not copy one hardening temperature across every 420-type grade
Published heat-treatment ranges vary across Type 420, JIS 420 variants, European martensitic grades and producer-specific blade steels. Even materials marketed within the broader “420” family can use materially different hardening temperatures and tempering recommendations.
For that reason, a purchasing article should not present one austenitizing temperature as a universal recipe. The correct source is the governing material specification or the steelmaker’s datasheet for the exact alloy being purchased.

Hardness should be specified as an acceptance requirement, not a marketing claim
Properly heat-treated 420-family steels can reach high Rockwell C hardness, but the attainable value varies substantially with carbon level and process. Some 420-type commercial alloys are designed around hardness in the high-40s to low-50s HRC range; higher-carbon martensitic variants may target different ranges.
The buyer should therefore define a permitted HRC window rather than request “maximum hardness.” Too much hardness can create brittleness, edge chipping, assembly cracking or poor toughness. A useful drawing requirement also identifies the hardness test method, test location, sampling quantity and whether the value applies before or after grinding and finishing.
304 uses solution annealing, not martensitic hardening
304 is normally supplied in a solution-annealed or controlled cold-worked condition. Solution annealing restores ductility and corrosion performance, but quenching after solution annealing does not transform 304 into a hard martensitic condition like 420.
304 can become much stronger through cold work, particularly in strip and formed products. Yet cold-worked 304 should be selected for applications where its strain-hardening behavior is useful—not as a shortcut for a blade, cutting edge or hard wear surface.
Mechanical Properties: Compare Condition-to-Condition, Not Grade-to-Grade
A single “420 vs 304 tensile strength” table can mislead because the condition often changes the result more than the grade name. Annealed 420, hardened-and-tempered 420, annealed 304 and heavily cold-worked 304 are four different mechanical states.
| Material / Condition | Hardness / Strength Profile | Ductility / Toughness Profile | Typical Procurement Purpose |
|---|---|---|---|
| 420 annealed | Relatively soft for machining | Higher ductility than hardened condition | Machine first, then harden and finish. |
| 420 hardened and tempered | High hardness and high strength | Reduced ductility; toughness depends on tempering | Blades, wear parts, shafts, valve trim and hard components. |
| 304 annealed | Moderate strength, relatively low hardness | Very high ductility and strong toughness | Deep drawing, welding, tanks, panels and general fabrication. |
| 304 cold worked | Strength and hardness can increase substantially | Ductility decreases as cold work increases | Spring-like strip, formed components and strength-enhanced products. |
Hardness and wear are related—but not identical
Higher hardness often improves resistance to abrasive or adhesive wear, but wear life also depends on counterface material, lubrication, contact pressure, surface roughness, microstructure, retained carbides and the type of motion. Therefore, specifying HRC alone does not guarantee a wear-life target.
Toughness can become the hidden design constraint
A high-hardness 420 part may perform well under controlled cutting or sliding conditions yet fail by chipping or cracking under impact. If the application combines high load, shock and corrosion, grades such as 431, 17-4PH or another engineered stainless solution may offer a more useful balance.
Corrosion Resistance: Why 304 Usually Has the Larger General-Service Margin
420 is stainless—but its corrosion behavior is more condition-sensitive
Martensitic 420 contains enough chromium to form a passive film and can provide useful corrosion resistance in mild environments. However, its higher carbon content and lower chromium level relative to common 304 mean that heat-treatment condition, carbide distribution, tempering, surface finish, contamination and passivation can strongly influence actual performance.
A correctly heat-treated and polished 420 component may work well in dry indoor use, cutlery, tools, light freshwater exposure or controlled environments. But “stainless” should not be interpreted as “maintenance-free” or “equivalent to 304 in wet service.”
304 is a stronger starting point for general wet fabrication
304 is widely selected for food equipment, vessels, kitchens, architectural components, appliances and general process fabrication because it combines corrosion resistance with high ductility, strong weldability and good surface cleanability.

Neither grade should be treated as a severe-chloride solution
304 can pit or suffer crevice corrosion in chloride-bearing environments, and ordinary 420 generally provides less corrosion margin than 304. For coastal salt, chloride cleaners, brackish water or more aggressive process conditions, the material review should move toward 316L stainless steel, duplex stainless steel or another higher-alloy material.
If the requirement combines hard mechanical properties with a severe corrosive environment, simply switching from 420 to 304 may solve corrosion but destroy the hardness requirement. This is a classic signal that the project needs a different alloy family rather than a compromise between the two original choices.
Surface condition can make a correct grade appear to be wrong
Carbon-steel grinding dust, contaminated polishing belts, free iron from handling equipment, scale, heat tint, rough machining and inadequate cleaning can all increase rust staining or localized attack. Critical parts should therefore use stainless-dedicated tooling and an appropriate cleaning/passivation process.
Fabrication Comparison: Machining, Forming, Welding and Polishing
| Process | 420 | 304 | Buyer Implication |
|---|---|---|---|
| Machining | Usually best before final hardening | Machinable but prone to work hardening | Define whether stock is supplied annealed and who performs final heat treatment. |
| Deep drawing | Limited compared with 304 | Excellent | Complex sheet shells usually favor 304. |
| Bending / forming | More condition-sensitive | Excellent in annealed condition | Do not form hardened 420 as if it were annealed sheet. |
| Welding | Requires tighter control; hard HAZ and cracking risk must be considered | Excellent general weldability | Heavy welded fabrication normally favors 304L/316L. |
| Polishing | Can achieve excellent hard polished surfaces | Widely available in decorative and sanitary finishes | Specify roughness or appearance standard instead of only “polished.” |
| Passivation | Useful, but process must suit the martensitic grade and heat-treated surface | Commonly used after fabrication | Cleaning before passivation is essential for both grades. |
420 is often machined first and hardened later
Machining a fully hardened martensitic component can require more expensive tooling and grinding. A common production strategy is to rough-machine in the annealed condition, leave an appropriate finishing allowance, heat treat, then grind or polish critical dimensions after hardening.
That sequence creates procurement questions that do not exist in a simple 304 sheet order: Who owns distortion after heat treatment? Is straightening permitted? Which dimensions are inspected before and after hardening? Is decarburization controlled? Is hardness tested on the finished part or a coupon?
304 welding is much more forgiving
Austenitic 304 is readily welded by common stainless-steel processes. For corrosion-critical welded fabrication, 304L is frequently preferred because lower carbon reduces sensitization risk in the heat-affected zone. See TISCO’s 304L stainless steel coil page for the low-carbon grade family.
“Polished” is not a measurable finish specification
Blade, mold, food and decorative applications use the word “polished” for very different surfaces. The RFQ should identify grit sequence, roughness target (Ra) where relevant, visual standard, directionality, mirror requirement, edge polishing and whether the finish is applied before or after heat treatment.
For additional finish control, review TISCO’s stainless steel polishing guide.
Application Selection Matrix: Where 420, 304 or Another Grade Makes Sense
| Application | Starting Material | Dominant Requirement | Key Procurement Control | Possible Upgrade |
|---|---|---|---|---|
| Knife / blade / cutting edge | 420-family or higher-carbon martensitic grade | Hardness and edge retention | Exact grade, heat treatment, HRC, edge geometry | 440-series or application-specific blade steel |
| Scissors / shears | 420-family depending design | Hard edge plus adequate toughness | Hardness uniformity, flatness and final grinding | Higher-carbon martensitic grade |
| Surgical cutting instrument | Martensitic instrument grade | Cutting performance, corrosion and sterilization | Applicable medical material standard, hardness and finish | Specialty martensitic grade |
| Medical tray / non-cutting hospital equipment | 304 / 316L depending environment | Cleanability and corrosion | Surface finish, welding, passivation and documentation | 316L |
| Mold cavity / corrosion-resistant tooling | 420-type mold steel where appropriate | Hardness, polishability and corrosion | Tool-steel quality, hardness, ESR/remelting requirement if needed | 1.2083, 1.2316, S136-type mold grade |
| Shaft / valve trim / wear component | 420 as a starting point | Wear plus moderate corrosion | HRC, runout, surface roughness and corrosion environment | 431 or 17-4PH |
| Food-processing frame / tank / panel | 304L | Welding, hygiene and general corrosion | Finish, weld quality, cleaning and MTC | 316L for more aggressive service |
| Kitchen sink / deep-drawn shell | 304 | Deep drawing and corrosion | Forming quality, thickness tolerance and surface | Application-dependent 304 variant |
| Architectural or appliance panel | 304 | Appearance, forming and corrosion | Finish, film, flatness and surface acceptance | 316L for coastal exposure |
| Hot chloride / marine wear component | Neither by default | Hardness plus severe corrosion | Full engineering material review | PH, duplex, super duplex, cobalt/nickel or coated solution depending service |
Blades: the word “420” still leaves unanswered questions
A blade needs more than a stainless grade. Edge angle, stock thickness, carbide population, heat treatment, hardness uniformity, grinding burn, straightness and final surface all influence cutting performance. Low-cost blade sourcing often fails because the buyer specifies a material name but not the finished edge performance.

Mold tooling: distinguish stainless mold steel from commodity 420 stock
Mold applications may require cleanliness, polishability, carbide control, ultrasonic quality, remelting practice, hardness uniformity and predictable heat-treatment response beyond what a commodity bar or plate specification guarantees.

One machine can legitimately use both 420 and 304
A food slicer is a good example. Its cutting blade may need hardened martensitic stainless, while the welded frame, guards, hopper and wash-down surfaces may be 304L or 316L. Material selection should be made component by component rather than assigning one stainless grade to the entire assembly.
When Neither 420 nor 304 Is the Best Answer
Alternatives when 420 is not tough or corrosion-resistant enough
| Alternative | Why Consider It | Main Trade-Off |
|---|---|---|
| 410 | Lower hardness requirement and general martensitic stainless function | Lower hardness / wear capability than higher-carbon 420-type grades. |
| 416 | Machining productivity is dominant | Free-machining additions reduce corrosion and welding performance. |
| 431 | Higher toughness and stronger corrosion performance are needed in a martensitic grade | Different heat treatment, availability and price. |
| 440-series | Higher hardness / edge retention is required | Toughness, grinding and heat-treatment control become more demanding. |
| 17-4PH | High strength with better general corrosion resistance and controlled age hardening | Different strengthening mechanism, specification and cost structure. |
| 1.2083 / S136-type tooling grade | Mold polishability, tooling quality and corrosion are key | Tool-steel supply chain and quality requirements are more specialized. |
Alternatives when 304 lacks corrosion margin
| Alternative | Use It When | Buyer Note |
|---|---|---|
| 304L | Welded fabrication makes low carbon desirable | Confirm the governing standard and whether dual certification is acceptable. |
| 316L | Chlorides, coastal salt or more aggressive cleaning chemistry raise pitting risk | Molybdenum improves localized-corrosion resistance but is not a universal seawater solution. |
| 430 | Dry indoor cost-down service can accept ferritic behavior | Corrosion, forming and welding behavior differ from 304. |
| 2205 duplex | Higher strength and stronger chloride/SCC resistance are required | Welding and fabrication procedures must follow duplex-specific controls. |
Cost: Raw Material Price Is Only One Part of the Decision
304 contains significant nickel, so its raw-material price is exposed to nickel market movements. Ordinary 420 typically contains little nickel, which can make the base alloy cheaper per kilogram in some markets.
But that comparison can reverse at the finished-part level. A 420 component may require annealed stock, rough machining, hardening, tempering, straightening, finish grinding, hardness inspection, polishing and passivation. Heat-treatment distortion or cracking can also create scrap or rework.
| Cost Driver | 420 Component | 304 Component | Commercial Impact |
|---|---|---|---|
| Alloy raw material | Often lower nickel cost | Nickel-bearing alloy cost | 420 may look cheaper before processing. |
| Heat treatment | Often essential for final function | Usually not a hardening operation | 420 adds furnace, handling and inspection cost. |
| Finish machining / grinding | May be required after hardening | Often completed without a hardening cycle | Final geometry can drive 420 cost. |
| Scrap / distortion risk | Higher where heat treatment is poorly controlled | Usually lower for ordinary fabricated products | Reject rate belongs in total-cost analysis. |
| Availability | More form- and subgrade-dependent | Very widely stocked globally | 304 often provides broader size and finish availability. |
Therefore, compare cost per accepted finished component, not only cost per ton. If the requirement is a hardened shaft, buying 304 because the sheet price looks familiar does not reduce cost—it creates a nonfunctional part. If the requirement is a welded tank, using 420 to save nickel cost creates processing and corrosion problems that the application never needed.
Procurement Verification: How to Confirm the Material and Condition
For 420, chemistry verification and hardness verification are separate questions
A chemical analysis can confirm the alloy family, but it does not prove that the component received the correct hardening and tempering cycle. Conversely, an HRC result can prove final hardness but cannot prove the exact grade or carbon level.
Critical orders therefore need both identity and condition evidence: heat-number traceability and an MTC for chemistry, plus a hardness report or finished-part test for the heat-treated condition.
XRF can distinguish broad families, but it does not solve the 420 subgrade problem
Handheld XRF can readily identify elements such as chromium and nickel and therefore helps separate a nickel-bearing 304 family from a standard low-nickel 420 family. However, carbon is the main variable separating many martensitic 420 subgrades, and handheld XRF is not the appropriate instrument for measuring carbon.
If the purchase requirement depends on carbon—such as distinguishing a lower-carbon 420-family grade from a higher-carbon cutting grade—use heat-specific certificate data and, when direct verification is required, a carbon-capable technique such as spark OES or combustion analysis.
Magnet tests are screening tools, not acceptance tests
420 is normally magnetic. Annealed 304 is generally much less magnetic, but 304 can develop a magnetic response after cold working or deformation. A magnet can therefore suggest a metallurgical family, but it cannot establish chemistry, carbon content, heat treatment or conformity to a purchase specification.
What the purchase documentation should contain
Recommended Evidence Package
- Heat-number-traceable MTC, commonly EN 10204 3.1 where required.
- Exact grade / designation and governing product standard.
- Heat-treatment condition for 420.
- Rockwell hardness results and test method for hardness-critical components.
- OES / carbon analysis when carbon verification is contractually required.
- Dimensional inspection after final heat treatment and grinding.
- Surface-finish / roughness inspection where specified.
- Passivation or cleaning records when required.
- Traceability transferred through cutting, machining, heat treatment and repacking.
- Final packing photos for export orders when agreed.
Heat-treatment outsourcing creates an extra traceability checkpoint
If a bar supplier ships annealed 420 to a separate heat treater, the heat identity must remain connected to the component batch through machining, furnace loading, quenching, tempering and final inspection. The RFQ should define whether the material supplier, part manufacturer or buyer owns this chain of custody.
Copy-Ready RFQ Checklist for 420 and 304 Stainless Steel
RFQ checklist for a heat-treated 420 component
- Exact grade: Type 420 / SUS420J1 / SUS420J2 / EN grade / producer-specific grade.
- Standard: applicable ASTM, JIS, EN, GB or drawing specification.
- Product form: bar, plate, strip, sheet, billet, blank or finished part.
- Dimensions: diameter / thickness / width / length / drawing dimensions.
- Supply condition: annealed, hardened and tempered, or project-specific condition.
- Target hardness: HRC range, not “hard” or “knife grade.”
- Hardness method: required test method, sampling frequency and test location.
- Heat treatment responsibility: supplier, buyer or named subcontractor.
- Dimensional acceptance: tolerances after heat treatment and final grinding.
- Surface finish: machined, ground, polished, mirror, Ra target or visual reference.
- Corrosion environment: humidity, water, food contact, chemicals, chlorides, sterilization or outdoor exposure.
- Documentation: MTC, heat traceability, hardness report, OES/carbon test if required.
- Quantity and packing: pieces / kg / tons, export packing and labeling.
- Destination and trade terms: delivery location, port and Incoterm.
Sample RFQ: hardened 420 shaft
Please quote Type 420 martensitic stainless steel shafts to the attached drawing. Material shall be supplied with heat-number-traceable MTC. Final condition: hardened and tempered to 48–52 HRC, unless a different range is approved in writing. Please confirm heat-treatment route, hardness test method and sampling, final diameter/runout tolerance after heat treatment, surface roughness, passivation requirement, quantity, packing and delivery time.
Sample RFQ: 420J2 blade blank
Please quote JIS SUS420J2 blade blanks to the attached dimensions. Please confirm chemistry, annealed incoming condition, proposed hardening/tempering route, target finished hardness, flatness after heat treatment, grinding allowance, surface condition, MTC, hardness report, carbon verification capability and export packing.
RFQ checklist for 304 / 304L fabricated material
- Grade: 304, 304L or approved dual certification.
- Product standard: appropriate sheet, coil, plate, bar, pipe or tube specification.
- Dimensions and tolerances: thickness, width, length, OD, wall, flatness or drawing values.
- Surface finish: No.1, 2B, BA, No.4, HL, mirror or project-defined roughness.
- Processing: slitting, cut-to-length, laser cutting, bending, welding, polishing or film.
- Service environment: indoor/outdoor, cleaning chemicals, chlorides, food contact or process chemistry.
- Weld requirements: filler, purge, cleaning, pickling/passivation and inspection if applicable.
- Documentation: MTC, PMI, traceability and third-party inspection if required.
- Packing and logistics: surface protection, seaworthy packing, quantity, Incoterm and destination.
Sample RFQ: 304L sheet for welded food equipment
Please quote ASTM A240/A240M Type 304L stainless steel sheet, 2B finish, to the specified thickness × width × length for welded indoor food-processing equipment. Please confirm dimensional tolerances, surface protection, EN 10204 3.1 MTC, heat-number traceability, flatness, export packing and delivery schedule.
FAQ About 420 vs 304 Stainless Steel
Is 420 stainless steel better than 304?
No. 420 is better when hardness, wear resistance, heat-treated strength or edge retention dominates. 304 is better when corrosion resistance, welding, forming, toughness and cleanability dominate. The correct grade depends on the failure mode.
Which is harder, 420 or 304?
Properly hardened 420 can be much harder than annealed 304. 304 can strengthen through cold work but cannot be conventionally quench-hardened like 420.
Can 420 stainless steel reach 50 HRC?
Many suitable 420-family compositions can be processed into the high-40s or low-50s HRC range, but the result depends on exact carbon level, producer specification, section size and heat treatment. Do not assume every material sold as “420” will reach the same hardness.
Is 420 stainless steel more corrosion-resistant than 304?
Usually not in general wet service. 304 normally provides a larger general corrosion margin. 420 can provide useful corrosion resistance in mild conditions, but its heat treatment and surface condition are especially important.
Can 304 be used for knife blades?
304 can be formed into a blade-shaped part but is generally not selected for a conventional cutting edge because it does not provide the heat-treated hardness and edge retention expected from martensitic blade steels.
Can 420 be used for food contact?
420-family stainless steels are used in cutlery and food-cutting components, but suitability depends on the exact grade, heat treatment, surface finish, corrosion exposure and applicable food-contact requirements. A welded food-processing tank or frame normally points toward 304L or 316L instead.
Can 420 be welded?
Yes, but welding is more demanding than with 304 because martensitic hardening can occur in the heat-affected zone. Preheat, controlled welding procedure and post-weld thermal treatment may be necessary depending on the grade, section and service.
Why can a 420 part rust after heat treatment?
Possible causes include unsuitable heat treatment, surface scale, carbide effects, rough finish, free-iron contamination, poor cleaning/passivation or an environment that exceeds the grade’s corrosion capability. Grade identity alone does not guarantee the final surface condition.
Is 420 magnetic?
Yes, martensitic 420 is normally magnetic. However, magnetism is not a grade-certification test. Cold-worked 304 can also show some magnetic response.
What is the difference between 420J1 and 420J2?
They are different JIS martensitic grades with different carbon ranges and therefore different hardness potential. J2 is generally selected when greater hardness is required. The exact JIS specification should be used rather than treating both as generic “420.”
Is 420HC the same as Type 420?
“420HC” is commonly used to describe a higher-carbon 420-type material, especially in cutting products, but it is not a single universal chemistry across all producers. Require the producer’s specification, MTC and finished hardness rather than approving the name alone.
Can XRF confirm 420J2 or 420HC?
Not by itself. XRF can identify major alloying elements such as chromium and nickel, but carbon is central to differentiating many 420-family grades. Carbon-specific verification requires certificate evidence and, when needed, a carbon-capable analytical method.
Which grade is better for a shaft: 420 or 304?
If the shaft needs hardened wear surfaces, 420 may be the better starting point. If corrosion, welding or fabrication matters more than hardness, 304 may be more appropriate. High-load shafts may instead justify 431, 17-4PH or another engineering grade.
Which is cheaper, 420 or 304?
420 may have a lower raw alloy cost because ordinary 420 contains little nickel, but the finished component can cost more after heat treatment, grinding, hardness testing and distortion control. Compare finished-part cost rather than only price per kilogram.
Conclusion: Choose by Failure Mode and Final Condition
Choose 420 when the component must be heat treated to a defined hardness or when wear resistance, edge retention and hard strength justify the lower ductility and more demanding processing route.
Choose 304 or 304L when the application is dominated by welding, forming, cleanability, toughness and general corrosion resistance. It is the more practical family for tanks, panels, food equipment, appliances, architectural components and many welded structures.
If the design demands both high hardness and a corrosion environment beyond ordinary 420—or if 304 corrosion resistance is insufficient—do not force either grade into the project. Review 431, 440-series, 17-4PH, 316L, duplex or another application-specific stainless grade.
Finally, specify more than the grade name. For 420, include the exact designation, heat-treatment responsibility, final HRC, dimensions after heat treatment and verification method. For 304, include the correct product standard, condition, finish, welding requirements, service environment and certificate scope.
Related TISCO Guides and Product Pages
Official and Technical References
- ASTM A240/A240M — Chromium and Chromium-Nickel Stainless Steel Plate, Sheet and Strip
- ASTM A276/A276M-25 — Stainless Steel Bars and Shapes
- ASTM A666/A666M-24 — Annealed or Cold-Worked Austenitic Stainless Steel Sheet, Strip, Plate and Flat Bar
- ASTM A967/A967M-25 — Chemical Passivation Treatments for Stainless Steel Parts
- ASTM F899-23 — Wrought Stainless Steels for Surgical Instruments
- ASTM E18-25 — Rockwell Hardness of Metallic Materials
- World Stainless — Stainless Steel Categories, Grades and Product Forms
- Carpenter Technology — Type 420 Stainless Alloy Information
- Outokumpu — Core 304 / 4301 Stainless Steel
Final material approval should follow the current edition of the governing product standard, purchaser drawing, service environment, heat-treatment specification, finished hardness, dimensional acceptance and traceable inspection records. Producer datasheets should be used for exact heat-treatment parameters of the specific martensitic grade.